Somehow, despite having more than 35 years of experience with a soldering iron, I had never used solder paste, although I’d heard a lot about it. So I decided to fill that gap by reviewing a tube of one member of this large family: Best BS-706 solder paste.
If you’re interested in my first attempts at working with solder paste and what I thought of it, come on in.


I’d really like to try several different pastes side by side. I think that kind of review would be more interesting for readers and more informative for me. Maybe I’ll get around to it someday, but for now I have just one tube, so that’s what I’ll be experimenting with.

The paste arrived in a regular little bag, with a syringe-shaped tube inside.


For obvious reasons, weighing the paste separately from the tube is difficult, so I had to weigh the whole thing. The total weight is 35.6 grams, and the tube is about 100 mm long.


The store page lists the dimensions, and they’re more or less accurate.


The plunger opening is covered with a cap, but there’s no plunger included. I had to use a marker cap instead. It fits the diameter perfectly, with a little friction, but it’s a bit too short. Anyway, there’ll be a photo at the end of the review showing how it looks :)


The stated composition of the paste:
Tin - 99%
Copper - 0.7%
Silver - 0.3%
Melting point - 138 degrees Celsius
Volume - 10 cubic cm

The label also lists safety precautions. In short: don’t eat it, don’t get it in your eyes, and wash your hands after use.


Unfortunately, there’s no needle included. Unscrewing the cap reveals a fairly thick tube. The paste is very runny: I squeezed some out, and after a while it simply ran onto the table.


The basic idea behind solder paste is quite simple: a large number of microscopic solder balls are suspended in a special flux, forming a single mass. When heated, the flux helps wet the surfaces being joined, while the solder itself bonds them together.
The melting point depends on the solder alloy. This one is rated at 138 degrees and consists of tin (99%), copper (0.7%), and silver (0.3%). The BST328 paste from the same company has a melting point of 183 degrees and is made of tin (63%) and lead (37%).

To me, there seems to be too much flux in this paste, which makes it feel very runny. The flux is transparent and clearly visible in the photo.


For testing, I used an Aoyue-2738 compressor soldering station, which I’ve had for many years, and factory-made circuit boards.


First, I decided to experiment a little, or, as you might say, “get the hang of it.” Put more simply, I wanted to see what solder paste is actually like.
To do that, I applied a little paste to the board’s pads, using different amounts to see how they compared. I set the air temperature to about 250 degrees.
My first impression: the paste really is very runny. You need to set the airflow as low as possible, or the components get blown off the board. Also, the idea was that surface tension would automatically align the components, but for some reason that didn’t happen.


I tried a slightly different approach and simply smeared some paste onto the board. You can see its “sandy” texture here, by the way.
After heating, the component settled fairly straight, and the excess paste gathered into larger solder balls. I wasn’t too keen on the fact that the solder under the resistor also seemed to want to form balls.


Now for the actual tests.
First, I applied paste to four pads on the circuit board.


I set the temperature to 140 degrees.


Unfortunately, the temperature fluctuates quite a lot, from about 137 to 170 degrees. This happens because the airflow is very low and the heater is powerful. When the temperature drops, the controller switches the heater on, and the temperature quickly shoots up to 165–170 degrees, then gradually falls to 135–140.


Of course, it would be more accurate to measure the temperature at the solder joint, since it will be lower than the temperature of the air coming out of the station’s nozzle. But it would also be difficult to catch the right moment, so I decided to limit myself to comparing the air temperature set on the soldering station with the result I got. I tried to heat the pads without affecting the ones next to them.
From left to right: 140-150-160-170-180-200-210-220 degrees.
At 140-170 degrees, the paste simply spreads out; at 180 it starts to melt, and at 200-220 it melts properly.


For the second test, I simply applied a lot of paste to several pads and watched what happened after heating: would the pads all stick together, or separate as they should?
Overall, it did pretty well. Most of the solder ended up where it was supposed to, while the rest gathered into large balls.


Next, I soldered a couple of 1206 resistors. This also went pretty well, except that the airflow shifted the resistors again because the paste is so runny.
The flux is almost transparent, but after cleaning it off with alcohol, whitish marks remain, and the solder itself looks a little dull.


For comparison, here's the same resistor soldered with a regular soldering iron and the solder I usually use. The process goes like this: hold the component with tweezers, touch one pad with the solder-coated tip and tack it in place, then solder the second contact, and finally touch up the first one. It sounds like a long and awkward process, but it's actually quite simple. I first tack all the SMD components in place this way, then solder them all. Sometimes I use regular flux, which we call F-3.
The photo shows a good solder joint: it's mirror-like, and you can even make out a bit of my hand holding the camera in the reflection.


A better and more proper way to apply the paste is with a stencil. For this, I used a piece of plastic with holes cut into it.
At first, I thought about making a proper stencil with a laser engraver, but I didn't really need one, and making it just for this review would take quite a while, so I decided to make do with this.


Place the stencil, spread the paste over it, scrape off the excess with something flat, and you get paste applied to the board.
The film is a little uneven, which makes it look like there's not much paste. In fact, it came out level with the thickness of the plastic, about 0.5 mm.


Place the components. The paste ended up about as thick as the components themselves. They stay put well: I turned the board upside down without any trouble, and nothing fell off or shifted.
Heat it with the hot-air gun.
In the end, two components soldered almost perfectly, but one rotated 90 degrees :(
After that, I washed the board and then removed the soldered components. It was almost clean underneath, and if it weren't for the rotated component, I'd say the test was a success.


Video of the soldering attempts.
In the second test, the hot-air gun wasn't quite perpendicular to the board, so it started blowing the components away. It wasn't very convenient to film and heat at the same time, so I only noticed during filming, but I decided to keep the video.


I used several circuit boards and a bunch of SMD resistors for the tests. It wasn't very convenient to experiment further, since I had to use a new board each time, but I think this was a clear enough demonstration.
By the way, this photo shows the marker being used as a plunger for the syringe.


I can already hear the obvious question: what's with all the identical boards in the photos? A long time ago, I used to make power supplies to order. Since they were ordered often and with different specifications, I designed a universal board.
You can see one example here.


The same board could also be used to build more powerful power supplies, up to about 70-100 W, as I did here.


For a while, I even considered making kits for assembling power supplies like these, but experienced builders wouldn't be interested, and I wouldn't want to give beginners a kit that could expose them to mains voltage.



It's hard to draw any firm conclusions. I can't judge objectively because I have no experience working with solder paste, so I'll have to give my subjective opinion.
In some situations, the paste could be useful, for example, to make it easier to desolder “difficult” components by thinning the solder already on the board.
Personally, I didn't like how runny it is. You either have to hold the hot-air gun far from the board, which means heating a larger area, or set the compressor to a very low power.
But I did like that the paste holds components in place on the board before soldering, doesn't leave much residue afterward, and generally behaves pretty well. The tests also showed that the actual temperature for this paste is around 220 degrees, which is consistent with the composition used; the stated 138 degrees is an error.

Perhaps some of the more experienced readers can recommend good solder pastes and explain whether I might simply have been doing something wrong.
That’s all from me. I hope the review was useful. As always, I’ll be glad to hear your questions, advice, and comments.
$4.78
Go to store
This page was found when searching for:
паста паяльная 138 градусов или 187, 3, https://www.kirich.blog/obzory/radiolyubitelskoe/649-nebolshoy-obzor-payalnoy-pasty-bst-706, паяльная паста низкотемпературная отзывы, рейтинг паяльных паст 2021г, паста bst montagekit свойства и противопоказания, паста плавления 138 зачем?, припой 138 градусов отзывы, миксер для паяльной пасты, паста паяльная в тубе, среднетемператцрная паяльная паста, плотность паяльной пасты кт 706, паяльная паста amtech 138, gfzkmyfz gfcnf bst 706, gfzkmyfz gfcnf bst-706, best bst 328 производитель, паста bst 5g состав, припойная паста температурой 150, паяльные пасты с температурой плавления 150, amtech bst-706, низкотемпературная паяльная паста, подскажите как пользоваться паяльной пастой хупер 190ра, bst 328 отзывы, паяльная паста 150 градусов, низкотемпературная паяльная паста отзывы, паста для паяльника, паяльная паста, использование паяльной пасты, паста для паяния, паяльная паста отзывы

Questions and answers

At what temperature does Best BS-706 solder paste melt?

The label states 138 °C, but in the test the paste melted reliably with the station set to 200–220 °C. The author concludes its actual melting point is about 220 °C.

What composition and melting point are specified for Best BS-706?

The stated composition is 99% tin, 0.7% copper, and 0.3% silver, with a melting point of 138 °C. The author considers the stated temperature an error.

What did the author like and dislike about Best BS-706?

It holds components on the board before soldering and does not leave much residue. Its high fluidity means hot-air flow can shift components, making it awkward to use with a hot-air tool.

The figures from this review are in the measurement database: Other devices


Discounted products


You may be interested in


Discounted products


Support the project

All the content on the site and the advice are free, but we’d be grateful for your support of the project and the channel!

Discuss on the forumHave a question or some experience to share? Discuss the article with the author and readers: the forum is a convenient place to share schematics and photos.
Go to the forum

Only registered readers can comment. It takes a minute to sign up, and you can log in with the same account you use on the forum.

Log inRegister